The first point, then, is to effectively crush the gangue, the degree of fineness being regulated by the fineness of the gold itself. This being done, then comes the question of saving the gold. If the quartz be clean, and the gold unmixed with base metal, the difficulty is small. All that is required is to ensure that each particle of gold shall be taken up by the mercury. The main object is to arrest the gold at the earliest possible stage; therefore, if you are treating clean stone containing free gold, either coarse or fine, I advise the use of mercury in the boxes, for the reason that a considerable proportion of the gold will be caught thereby, and settling to the bottom, or adhering to amalgamated plates in the boxes, where such are used, will not be afterwards affected by the crushing action, which might otherwise break up, or “flour,” the mercury. On the whole, I rather favour the use of mercury in the box at any time, unless the ore is very refractory—that is, contains too great a proportion of base metals, particularly sulphides of iron, arsenic, &c., when the result will not be satisfactory, but may entail great loss by the escape of floured mercury carrying with it particles of gold. Intelligent experience will assist the battery manager to adopt the right system.

The crushed stuff—generally termed the “pulp”—passes from the boxes through the “screens” or “gratings,” and so on to the “tables”—i.e., sheets of copper amalgamated on the upper surface with mercury, and sometimes electroplated with silver and afterwards treated with mercury. Unless the quartz is very clean, and, consequently light, I am opposed to the form of stamper box with mercury troughs cast in the “lip,” nor do I think that a trough under the lip is a good arrangement, as it usually gets so choked and covered with the heavy clinging base metals as to make it almost impossible for the gold to come in contact with the mercury. It will be found better where the gold is fine, or the gangue contains much base metal, to run the pulp from the lip of the battery into a “distributor.”

The distributor is a wooden box the full width of the stamper box or mortar, having a perforated iron bottom set some three to four inches above the first copper plate, which should come up under the lip. The effect of this arrangement is that the pulp is dashed on to the plate by the falling water, and the gold at once coming in contact with the mercury begins to accumulate and attract that which follows, till the amalgam becomes piled in little crater-shaped mounds, and thus 75 per cent. of the gold is saved on the top plate.

I have tried a further adaptation of this process when treating ores containing a large percentage of iron oxide, where the bulk of the gold is impalpably fine, and contained in the “gossan.” At the end of the blanket table, or at any point where the crushed stuff last passes before going to the “tailings heap” or “sludge pit,” a “saver” is placed. The saver is a strong box about 15 in. square by 3 ft. high, one side of which is removable, but must fit tight. Nine slots are cut inside at 4 in. apart, and into these are fitted nine square perforated copper plates, having about eighty to a hundred ¼ in. holes in each; the perforations should not come opposite each other. These plates are to be amalgamated on both sides with mercury, and the top plate “fed” from time to time with mercury, in which a very little sodium has been placed. If acid ores are being treated, zinc should be employed in place of sodium, and to prevent the plates becoming bare, if the stuff is very poor, thick zinc amalgam may be used with good effect; but in that case discontinue the sodium, and occasionally, if required, say once or twice in the day, mix an ounce of sulphuric acid in a half gallon of water and slowly pour it into the launder above the saver. Underneath the “saver” you require a few riffles, or troughs, to catch any waste mercury, but if not overfed there should be no waste. This automatic appliance sometimes arrests a considerable quantity of gold.

We now come to the subsidiary processes of battery work, the “cleaning” of plates, and “scaling” same when it is desired to get all the gold off them, the cleaning and retorting of amalgam, and of the mercury, smelting gold, &c.

Plates should be tenderly treated, kept as smooth as possible, and when cleaning up after crushing, in your own battery, the amalgam—except, say, at half-yearly intervals—should be removed with a rubber only; the rubber is simply a square of black india-rubber or soft pine wood.

Fig. 23. Scraper.

When crushing rich ore, and you want to get nearly all the gold off your plates, the scraper [(Fig. 23)] may be resorted to. This is usually made by the mine blacksmith from an old flat file which is cut in half, the top turned over, beaten out to a sharp blade, and kept sharp by touching it up on the grinding-stone. This, if carefully used, will remove the bulk of the amalgam without injury to the plate.