"(b) (It is proposed to prescribe, under this paragraph, the requirements in regard to deflection, fixing maximum and minimum limits, as soon as proper deflection limits have been decided upon.)

Tests.

"13. (A) Two pieces shall be tested from each heat of steel. If either of these test pieces breaks, a third piece shall be tested. If two of the test pieces break without showing physical defect, all rails of the heat will be rejected absolutely. If two of the test pieces do not break, all rails of the heat will be accepted as No. 1 or No. 2 classification (according as the deflection is less or more, respectively, than the prescribed limit[F]).

"(B) If, however, any test piece broken under test A shows physical defect, the top rail from each ingot of that heat shall be rejected.

"(C) Additional tests shall then be made of test pieces selected by the Inspector from the top end of any second rails of the same heat. If two out of three of these second test pieces break, the remainder of the rails of the heat will also be rejected. If two out of three of these second test pieces do not break, the remainder of the rails of the heat will be accepted, provided they conform to the other requirements of these specifications, as No. 1 or No. 2 classification (according as the deflection is less or more, respectively, than the prescribed limit[F]).

"(D) If any test piece, test A, does not break, but when nicked and tested to destruction shows interior defect, the top rails from each ingot of that heat shall be rejected.

Drop testing machine.

"14. The drop-testing machine shall be the standard of the American Railway Engineering and Maintenance of Way Association, and have a tup of 2,000 lbs. weight, the striking face of which shall have a radius of five (5) in.

"The anvil block shall be adequately supported and shall weigh 20,000 lbs.

"The supports shall be a part of or firmly secured to the anvil.