Fig. 4.

Locomotive, 90 lbs. Sketch shows interior view of fire-box with front removed. The left side of the copper fire-box burst inwards owing to the plate in line of fracture being corroded to less than 1/8 inch.

No.6. Stoke. ([Fig. 5.])

February 6th.

none injured.

Fig. 5.

One of three. One tube Cornish, with two external fire grates with a water tube over each fire. It was 30ft. 2in. long, 6ft. diameter. Tube 3ft. diameter, 3/8 inch plates, 40 lbs. pressure. External shell is shown in dotted lines to allow of the tubes being seen. The tube had formerly been placed rather higher in the boiler. The tube collapsed sideways, having become overheated from shortness of water. The boiler itself was but little disturbed.

No.7. Kelso. ([Fig. 6.])