FIG. 21.—Cutting up barrels.

FIG. 22.—Upsetting the ends.

The stock, which came in bars of mill length, was cut off so as to make a barrel with the proper allowances for trimming (Fig. 21). They then pass to the forging or upsetting press in the adjoining room. This press, which is shown in more detail in Fig. 22, handled the barrels from all the heating furnaces shown. The men changed work at frequent intervals, to avoid excessive fatigue.

FIG. 23.—Continuous heating furnace.

Then the barrels were reheated in the continuous furnace, shown in Fig. 23, and straightened before being tested.

The barrels were next tested for straightness. After the heat-treating, the ends are ground, a spot ground on the enlarged end and each barrel tested on a Brinell machine. The pressure used is 3,000 kg., or 6,614 lb., on a 10-millimeter ball, which is standard. Hardness of 240 was desired.

The heat-treating of the rifle blanks covered four separate operations: (1) Heating and soaking the steel above the critical temperature and quenching in oil to harden the steel through to the center; (2) reheating for drawing of temper for the purpose of meeting the physical specifications; (3) reheating to meet the machine ability test for production purposes; and (4) reheating to straighten the blanks while hot.